TCP Global

SEEDINESS

Grainy, Speckled, Gritty, Dirty

Solid particles of various shapes and sizes embedded evenly throughout the paint film.

CAUSE

    Material not properly stirred or agitated.
  • Failure to strain material.
  • Using material exceeding its shelf life.
  • Using generic reducers and/or hardeners.
  • Using materials beyond their specified pot life.
  • Using contaminated thinner/reducer or hardener.
  • Using contaminated water borne products.

REPAIR

Remove the wet paint film with solvent, clean and refinish.

Or, sand smooth and refinish.

PREVENTION

  • Stir or shake materials thoroughly to be sure all pigment/resin is in solution.
  • Strain all undercoats and topcoats.
  • Do not use material that cannot be stirred or strained. Caution: Repeated straining will not completely remove seediness.
  • Use the recommended thinner/reducer and hardener, and then measure accurately.
  • Mix only enough material that can be used within specified pot life.
  • Use material as soon as possible, close and tighten container lids immediately after use.
  • Do not allow thinner/reducer to come into contact with water borne products.